H06-1
YMS
7-15days
200kg
10T/day
Shanghai,Qingdao,Guangzhou,Ningbo etc
Gray
No Gloss
~1.92Kg/L (after mixing)
27℃
(45±2 )%
Use the power mixer to mix the main paint evenly, and then add the hardener and stir until it is well mixed. Generally, if the temperature below 10℃, it needs 30 min induction time; if the temperature over 10℃, it needs 15 min induction time.
Part A: Part B= 30:3 (by weight)
2.93m²/Kg (80um dry film thickness)
| Availability: | |
|---|---|
This two-component product is mainly prepared by epoxy resin, ultra-fine zinc powder, and polyamide as curing agent. This product features:
 
  |   
  |   
  |  
 
  |   
  |   
  |  
Appearance  |  Grey, matt  |  
Density, kg/L  |  ~2.30  |  
Flash point, ℃  |  Part A: 24 Part B: 27  |  
Zinc content  |  ≥ 60 %  |  
Impact resistance, cm  |  50 | 
Adhesion, MPa  |  ≥6 | 
Pot life, h @ 23 ± 2 ℃  |  ≥5 | 
Theoretical spreading rate, kg/m2 @ 80 µm dry film  |  0.3 | 
VOC, g/L  |  420 | 
![]()  |  H06- 1 Epoxy Zinc-rich Primer Product PackagingPackaging: Part A: 30 kg in a 20-liter iron barrel Part B: 3 kg in a 5-liter iron barrel. Shelf Life: Part A: 12 months Part B: 12 months If exceeding shelf life, the products shall be tested before using.  |  
Applicable Environment
![]()  |  ![]()  |  ![]()  |  ![]()  |  
Boat  |  gas storage tank  |  oil storage tank  |  galvanized workpiece  |  
![]()  |  ![]()  |  ![]()  |  ![]()  |  
Offshore platform  |  Iron tower  |  Shipyard  |  Bridge  |  
Compatibility
| Product | Thickness | |
| Primer: | H06- 1 Epoxy Zinc Rich Primer | 2*40 µm  |  
| Midcoat: | H53-6 Epoxy Mica Iron Oxide Paint  |  150 µm  |  
| Topcoat: | BS52-10 Acrylic Polyurethane Finish Paint  |  2*40 µm | 
Finished Projects
![]()  |  ![]()  |  ![]()  |  
Production Process
![]()  |  ![]()  |  ![]()  |  
H06- 1 Epoxy Zinc-rich Primer
Instructions For Use
Substrate Treatment:
All surface shall be clean, dry and free from any contaminations to achieve long lasting function.
Carbon Steel
Minimum St 3 (ISO 8501-1)
Optimum Sa 2½ (ISO 8501- 1)
Primed steel
Blasted to Sa 2 (ISO 8501- 1)
Instructions for Use:
Mixing
Mix part A and part B as 30:3 by weight. Slowly add part B into part A and ensure mixed completely.
Thinner
X-7 Epoxy paint thinner ≤ 10 % w./w.
Cleaner
X-7 Epoxy paint thinner
Application methods:
Airless spray (recommended): Nozzle tip: 0.015-0.021 inch, minimum 150 bar/2100 psi
Brush: recommended for small areas only.
Roller: recommended for small areas only.
Company Introduction
![]()  |  |||
![]()  |  ![]()  |  ![]()  |  ![]()  |  
Exhibitions
![]()  |  ![]()  |  ![]()  |  
![]()  |  ![]()  |  ![]()  |  
This two-component product is mainly prepared by epoxy resin, ultra-fine zinc powder, and polyamide as curing agent. This product features:
 
  |   
  |   
  |  
 
  |   
  |   
  |  
Appearance  |  Grey, matt  |  
Density, kg/L  |  ~2.30  |  
Flash point, ℃  |  Part A: 24 Part B: 27  |  
Zinc content  |  ≥ 60 %  |  
Impact resistance, cm  |  50 | 
Adhesion, MPa  |  ≥6 | 
Pot life, h @ 23 ± 2 ℃  |  ≥5 | 
Theoretical spreading rate, kg/m2 @ 80 µm dry film  |  0.3 | 
VOC, g/L  |  420 | 
![]()  |  H06- 1 Epoxy Zinc-rich Primer Product PackagingPackaging: Part A: 30 kg in a 20-liter iron barrel Part B: 3 kg in a 5-liter iron barrel. Shelf Life: Part A: 12 months Part B: 12 months If exceeding shelf life, the products shall be tested before using.  |  
Applicable Environment
![]()  |  ![]()  |  ![]()  |  ![]()  |  
Boat  |  gas storage tank  |  oil storage tank  |  galvanized workpiece  |  
![]()  |  ![]()  |  ![]()  |  ![]()  |  
Offshore platform  |  Iron tower  |  Shipyard  |  Bridge  |  
Compatibility
| Product | Thickness | |
| Primer: | H06- 1 Epoxy Zinc Rich Primer | 2*40 µm  |  
| Midcoat: | H53-6 Epoxy Mica Iron Oxide Paint  |  150 µm  |  
| Topcoat: | BS52-10 Acrylic Polyurethane Finish Paint  |  2*40 µm | 
Finished Projects
![]()  |  ![]()  |  ![]()  |  
Production Process
![]()  |  ![]()  |  ![]()  |  
H06- 1 Epoxy Zinc-rich Primer
Instructions For Use
Substrate Treatment:
All surface shall be clean, dry and free from any contaminations to achieve long lasting function.
Carbon Steel
Minimum St 3 (ISO 8501-1)
Optimum Sa 2½ (ISO 8501- 1)
Primed steel
Blasted to Sa 2 (ISO 8501- 1)
Instructions for Use:
Mixing
Mix part A and part B as 30:3 by weight. Slowly add part B into part A and ensure mixed completely.
Thinner
X-7 Epoxy paint thinner ≤ 10 % w./w.
Cleaner
X-7 Epoxy paint thinner
Application methods:
Airless spray (recommended): Nozzle tip: 0.015-0.021 inch, minimum 150 bar/2100 psi